| | | NINGBO EAST MAGNET CO.,LTD. | | |
| | | |
| | | sffiussndfebttttflg* Magnetic Properties of Compression Moulding Bonded NdFeB Magnet | | |
| | | |
| | | | | | | | | | | | | | | | | | | | | | mb Rcmanencc | Coercive Force | Intrinsic Coercive Force | Max. Energy Producl | Recoil Temp. | Max. Working Temp. | tea Density | | | | Grade | Br | | Heb | He | | ( BH | 1 Max | Permeability | vocnieicni a(Brl | | | | | | T | KGs | kA/m | kOe | kA/m | kOe | kj/m' | MGOe | _m_ | %IK | ■fc | g/cm' | | | | | | | | | | | | | | BNP-6 | 0.55-0.62 | 5.5-6.2 | 285-370 | 3.6-4.6 | fitXt-755 | 7.5-9.5 | 44-56 | 5.5-7 | 1.15 | -0.13 | 100 | 5.5-6.1 | | | | BNP-8l | 0.60-0.64 | 6.0-6.4 | 360-400 | 4.5-5.0 | 715-HIMi | 9-10 | 56-64 | 7.0-8.0 | 1.15 | -0.13 | too | 5.6-6.1 | | | | BNP-8 | 0.62—0.69 | 6.2-6.9 | 385-445 | 4.8-5.6 | 640-800 | 8-10 | 64-72 | 8.0-9.0 | 1.15 | -0.13 | 120 | 5.8-6.1 | | | | BNP-8sr | 0.62-0.66 | 6.2-6.6 | 410-465 | 5.2-5.8 | 880-1120 | 11-14 | 64-72 | 8.0-9.0 | 1.13 | -0.13 | ISO | 5.8-6.1 | | | | BNP-8h | 0.61-0.65 | 6.1-6.5 | 410-455 | 5.2-5.7 | II'Ml-1440 | 15-ia | 64-72 | 8.0-9.0 | 1.15 | -0.07 | 125 | 5.9-6.2 | | | | BNP-9 | 0.65-0.70 | 6.S-7.0 | 40O-44O | 5.0-5.5 | 640-800 | 8-10 | 70-76 | 8.8-9.5 | 1.22 | -».12 | 120 | 5.8-6.1 | | | | BNP-10 | 0.68-0.72 | 6.8-7.2 | 420-47O | 5.3-5.9 | 640-800 | K— III | 76-84 | 9.5-10.5 | 1.22 | -0,11 | 120 | 5.8-6.1 | | | | BNP-11 | 0.70-0.74 | 7.0-7.4 | 445-480 | 5,6-6.0 | 68Ö-8O0 | 8.5-10 | 80-88 | 10.0-11.0 | 1.22 | -r>.11 | 120 | 5.8-6.1 | | | | BNP-IIL | 0.70-0.74 | 7.0-7.4 | 4181-440 | 5.0-5.5 | 520-440 | 6.5-8 | 78-84 | 9.8-10.5 | 1.26 | -0.11 | no | 5.8-6.1 | | | | BNP-i2l | 0.74-0.80 | 7.4-8.0 | 420-455 | 5.3-5.7 | 520-000 | 6.5-7.5 | 84-92 | 10.5-11.5 | 1.26 | -0.O8 | 110 | 5.8-6.1 | | | | | | | | | | | | | | | | | | | | |
| | | |
| | | Notes: The properties given above are typical .it room iemperature(2.Vt") for umojtcd samples. | | |
| | | |
| | | sltjft9ndfeb{sttl№le Magnetic Properties of Injection Moulding Bonded NdFeB Magnet Mts *«» w«»«7i «*bis» sjiSBS* äiaasBR utaa »a | | |
| | | |
| | | | | | | | | | | | | | | | | | | | | | Remancnce | Coercive Force | Intrinsic Coercive Force | Max. Energy Product | Recoil Permeability | Temp. Coefficient a(Br) | Max. Working Temp. | Density | | | | Grade | Br | | Heb | Hcj | 1 BH | 1 Max | | | | | | T | KGs | kA/m | kOe | kA/m | kOe | KJ/m' | MGOe | | %/t | | fl/cm' | | | | BNI-3 BNI-4 BNI-5 | 0.2-0.4 11.40-0.46 0.45-0.51 | 2.0-4.0 4.0-4.8 4.5-5. 1 | 120-210 250-335 280-360 | 1.5-3.0 3.1-4.2 3.5-4.5 | 480-640 575-735 640-800 | 6.0-8.0 7.2-9.2 8-10 | 8-24 28-36 37-44 | 1.0-3.0 3.5-4.5 4.6-5.5 | 1.2 1.2 | -0.15 -0.13 -0.13 | too no 120 | 3.9-4.4 4.2-4.9 4.5-5.0 | | | | | | | | BNI-6 | 0.51-0.56 | 5. 1-5.6 | 295-375 | 3.7-4.7 | 640-8181 | 8-10 | 44-52 | 5.5-6.5 | 1.13 | -0.11 | 120 | 4.7-5.1 | | | | BNI-6h | 0.48-0.56 | 4.8-5.6 | 335-400 | 4.2-5.0 | 1035-1355 | 13-17 | 40-52 | 5.0-6.5 | 1.13 | -0,15 | 130 | 4.8-5.2 | | | | BNI-7 | 0.54-0.64 | 5.4-6.4 | 320-400 | 4.0-5.0 | 640-800 | 8-10 | 51-59 | 6.5-7.5 | 1.13 | -0.11 | 120 | 5.0-5.5 | | | | BNI-SSR(PPS) | 0.45-0.50 | 4.5-5.0 | 300-360 | 3.8-4.5 | 875-1115 | 11-14 | 36-44 | 4.5-5,5 | 1.13 | -0.13 | 150 | 4.9-5 4 | | | | | | | | | | | | | | | | | | | | |
| | | |
| | | it: Bti.tt#tt*5s(a(2w3äm. mmammikWiM Notes: The properties given ahovc arc typical at mom tcmpcraturc(2.Vt'.) for uncoatcd sample* | | |
| | | |
| | | 07 | | |
| | | |
| | | | | | | | | | | | | | | |