Polyamide and Polyethyleneterephthalate Fi ben
Fi ber-rein forced Polymer Composite
the spinning process of the frbers Fiber no I (PA 66) is comparably free of stress Heating rate: 10 K/min load 10 g, static
The difference m the thermally induced expansion of a fiber-reinforced polymer composite is shown here with measurements in the perpendicular and longitudinal direction
This composite is used in the manufacture of brake linings The reason for the increased expansion of the perpendicular sample is reduced strength between fiber layers
Before melnng. libera no 2 (PA 612) and no 3<P£D show a considerable shrink­age due to stress relaxation This stress is induced during
IMu
A special sample carrier is necessary for measuring the expansion during melting and the contraction during solidification of waxes The change in volume of a wax sample o' low viscosity being used for investment
(10 g] and a heating rate of S K/mm These differences are caused by varied copolymerizalion with other
Three different colored PMMA samples show considerable differences m Ih* viscoelastic range above 100 "C ai oscillating load
-.'■-■I.
hysteresis during cooling The relative change in length as a value for the sample vdume was measured at a healing rale of 2 K/mm and load of 0 3 g
DirectIndustry's Virtual Technical Library: PDF Catalogue | Technical Documentation | Brochure | Manual | Industrial directory | Specifications | Characteristics
Search Go
page 1 p.1
page 2 p.2
page 3 p.3
page 4 p.4
page 5 p.5
page 6 p.6
page 7 p.7
page 8 p.8
pdf-page pdf di En 2008-11-47-23